Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the translatepress-multilingual domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home1/sohoweld/public_html/waldunsteel/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the wordpress-seo domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home1/sohoweld/public_html/waldunsteel/wp-includes/functions.php on line 6114
35NiCr6 / 1,5815 Aço - EN 10083 | Waldun Steel

35NiCr6 / 1.5815 Aço

35NiCr6 1,5815 Aço

35NiCr6 / 1.5815 Aço Descrição

Liga de aço especial O aço de grau 35NiCr6 pertence aos aços-liga para têmpera e revenimento. O material não. é 1,5815.

35NiCr6 / 1.5815 Aço Inscrição

Aço para melhoramento térmico caracterizado por propriedades de alta resistência, boa ductilidade, resistência à fadiga e ao impacto. Usado para peças pesadas de motores, dispositivos e máquinas, usado na produção de virabrequins, engrenagens, eixos, hastes de pistão, parafusos, engrenagens tratadas termicamente e hastes de pistão.

  • Virabrequins.
    • Veios.
    • Várias engrenagens.
    • Fixadores etc

35NiCr6 / 1.5815 Aço Comparação de todas as notas

DIN EN ANFOR AECMA
1,5815 35NiCr6 35NC6 FE-PL62

35NiCr6 / 1.5815 Aço Padrão de qualidade

EN 10083 Aços para têmpera e revenido. Condições técnicas de entrega para aços de liga
EN 10250 Forjados de aço aberto para fins de engenharia em geral. Aços especiais de liga

35NiCr6 / 1.5815 Aço Composição Química de acordo com EN 10083-3

NOTA NÚMERO C Si Mn P S Cr Ni
35NiCr6 1,5815 0,30-0,37 ≤ 0,40 0,60-0,90 ≤ 0,025 ≤ 0,025 0,80-1,10 1,20-1,60

35NiCr6 / 1.5815 Aço Propriedades Mecânicas (T = 20 ° C se não for declarado de forma diferente)

Processar Diâmetro (mm) Resistência à tração Rm (Mpa) Força de rendimento Rp0,2 (Mpa) Alongamento A5 (%) Razão de redução de área C (%) Valor de impacto Kv (J) Temperatura ambiente Dureza (HB)
SOFT ANNEALED / / / / / / 223 max
TEMPERADO E REVENIDO 16 máx. 880-1080 740 min 12 min 40 min / 261-318
TEMPERADO E REVENIDO 16-40 880-1080 740 min 12 min 40 min 35 min 261-318
TEMPERADO E REVENIDO 40-100 780-980 640 min 15 min 40 min 35 min 231-289

35NiCr6 / 1.5815 Aço TRATAMENTO TÉRMICO:

Processar TEMPERATURA ° C Meio de resfriamento
Deformação plástica quente 850-1100 /
Normalização 850-880 ar
Recozimento suave 640-690 ar
Endurecimento 840-860 óleo
Temperamento 530-630 ar

35NiCr6 / 1.5815 Aço Certificado de teste de Mill: