Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the translatepress-multilingual domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home1/sohoweld/public_html/waldunsteel/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the wordpress-seo domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /home1/sohoweld/public_html/waldunsteel/wp-includes/functions.php on line 6114
30NiCrMo16-6 / 1.6747 Aço - EN 10083 | Waldun Steel

30NiCrMo16-6 / 1.6747 Aço

30NiCrMo16-6 1.6747 Aço

30NiCrMo16-6 Aço para têmpera e têmpera 1.6747 35NCD16

30NiCrMo16-6 / 1.6747 Steeeu Inscrição

30NiCrMo16-6 / 1.6747 O aço apresenta ótima temperabilidade, resistência ao impacto, carga, deformação, resistência ao desgaste e tensões.

Usado para peças pesadas de motores, dispositivos e máquinas, indústrias de aviação e aeroespacial, usado na produção de virabrequins, engrenagens, eixos, parafusos, engrenagens tratadas termicamente e hastes de pistão, etc.

30NiCrMo16-6 / 1.6747 Aço Padrão de qualidade

-DIN EN 10083-3 Aço para têmpera e têmpera de aços-liga.

30NiCrMo16-6 / 1.6747 Aço Composição Química de acordo com EN 10083-3

NOTA NÚMERO C Si Mn P S Cr Mo Ni
30NiCrMo16-6 1,6747 0,26-0,33 ≤ 0,40 0,50-0,80 ≤ 0,025 ≤ 0,025 1,20-1,50 0,30-0,60 3h30-4h30

 

30NiCrMo16-6 / 1.6747 Aço Propriedades mecânicas

Tratamento térmico Diâmetro
(milímetros)
Resistência à tração Rm (Mpa) Força de rendimento Rp0,2 (Mpa) Alongamento % em 2 ″ (%) Redução de área (%) Teste de impacto
(J)
Q + T 16 máx. 1080-1230 880 min 10 min 45 min /
Q + T 16-40 1080-1230 880 min 10 min 45 min 35 min
Q + T 40-100 1080-1230 880 min 10 min 45 min 35 min
Q + T 100-160 900-1050 790 min 11 min 50 min 35 min
Q + T 160-250 900-1050 880 min 11 min 50 min 35 min

30NiCrMo16-6 / 1.6747 Aço Tratamento térmico

Processar Temperatura
Normalizando o recozimento 850 - 880 ℃
Recozimento de amolecimento 650 - 700 ℃
Endurecimento 865 - 885 ℃
Temperamento 550 - 650 ℃
Dureza em estado amolecido 269 HB máx.

30NiCrMo16-6 / 1.6747 Aço Teste

Análises químicas, análises mecânicas, testes ultrassônicos, metalográficos, qualidade de superfície e relatório de dimensões.

30NiCrMo16-6 / 1.6747 Aço Certificado de teste de Mill

EN 10204 / 3.1 com todos os registros de dados relevantes. Chem. composição, mech. propriedades e resultados dos testes.

Produtos Mais recentes

ENTRE EM CONTATO COM A WALDUN STEEL

Móvel:

+8618652469606

O email:

iguhongtao@gmail.com

waldun aço iso 9001 logo 300x158

Faça uma cotação agora!

© Copyright - WALDUN STEEL